Plastic In. Metal Out. | Electroplating 3D Printed Parts for Metal Performance (Part 1) — Transcript

by MLC CAD Systems · 5,297 words · 787 segments · language en · Watch on YouTube

Full transcript

  1. 0:00This may look like an ordinary metal
  2. 0:02housing that was CNC machined, but what
  3. 0:05if I told you that the manufacturing
  4. 0:07process used to make this is the same as
  5. 0:11what was used to make this? And if
  6. 0:14that's not surprising enough, what if I
  7. 0:17also told you that both of these started
  8. 0:19out as 3D printed plastic parts?
  9. 0:23This conversion from plastic to metal is
  10. 0:26possible with electroplating. And in
  11. 0:29today's webinar, we'll expose you to one
  12. 0:31of the most powerful post-processing
  13. 0:34techniques available for your 3D prints.
  14. 0:41Electroplating is the process of using
  15. 0:43electricity and an electrolyte solution
  16. 0:46to transfer positive metal ions from one
  17. 0:49metal electrode like copper to another
  18. 0:52electrode, resulting in a thin metal
  19. 0:55coating. Traditionally, this other
  20. 0:58electrode is also made of metal because
  21. 1:01it's naturally conductive, but it
  22. 1:03doesn't have to be. Non-conductive
  23. 1:06substrates like plastic, can also be
  24. 1:09plated once an ultra thin conductive
  25. 1:12layer is applied. And plastic,
  26. 1:15particularly 3D printed plastic, is
  27. 1:18where you often see the most profound
  28. 1:20benefits of electroplating. When 3D
  29. 1:23printed plastic parts are electroplated,
  30. 1:26it creates a composite where the whole
  31. 1:28is truly greater than the sum of its
  32. 1:30parts. Thanks to the metal coating, the
  33. 1:33parts can be stiffer and more rigid,
  34. 1:37thermally and electrically conductive.
  35. 1:41They have improved aesthetics,
  36. 1:44and are vastly more resistant to harsh
  37. 1:47environments, to chemicals, and UV
  38. 1:51light. And the benefits don't stop there
  39. 1:53because with 3D printing, you have a
  40. 1:56lightweight plastic core and the ability
  41. 1:58to produce geometries impossible to
  42. 2:01manufacture traditionally.
  43. 2:03Lastly, thanks to the lowcost nature of
  44. 2:053D printing, using electroplating to
  45. 2:08achieve metal properties is often
  46. 2:10cheaper than casting or machining.
  47. 2:13It's easy to see how electroplating 3D
  48. 2:15printed parts can unlock applications
  49. 2:18into a wide variety of industries.
  50. 2:21To demonstrate this, we 3D printed nine
  51. 2:24different parts representing automotive,
  52. 2:27consumer products, maritime,
  53. 2:30entertainment, architecture, and
  54. 2:32electronics in addition to parts that
  55. 2:36illustrate electroplating's various
  56. 2:38superpowers.
  57. 2:40The decision to print these parts in
  58. 2:41gray V5, rigid 10K, and nylon 12 on our
  59. 2:45Formlabs printers, as well as
  60. 2:47understanding the different plating
  61. 2:49options available and the clearances
  62. 2:52that are needed to account for the
  63. 2:53different plating thicknesses could only
  64. 2:56happen thanks to the expert guidance at
  65. 2:58Repl. Having electroplated 3D printed
  66. 3:02parts for customers in nearly every
  67. 3:04industry for over 25 years, they have
  68. 3:06easily earned the title of masters of
  69. 3:09their craft. I met with Repl's president
  70. 3:12and founder, Dr. Sha Weiss, and
  71. 3:15extracted some important excerpts from
  72. 3:17our conversation.
  73. 3:19>> I'm Sean Weise. I'm the president of
  74. 3:20Replform. The company's been established
  75. 3:22for 26 years. I've been electroplating
  76. 3:26on additive manufactured parts since the
  77. 3:29mid mid to early 90s. [snorts] So more
  78. 3:32than 30 years. When I started out, I was
  79. 3:35making electroforms that were a tenth of
  80. 3:37an inch thick. So not really bending
  81. 3:39metal, but creating shapes um that way
  82. 3:42off of SLA patterns. Now most of the
  83. 3:44coating that we do is anywhere between
  84. 3:4620,000 and 6,000 of an inch. So we work
  85. 3:50at much much thinner layers. Plus the
  86. 3:52the parts that people print are
  87. 3:54generally, you know, an eighth of an
  88. 3:55inch or less for wall thickness. Not
  89. 3:57always the case, but um we can reinforce
  90. 4:00those parts with the plating because the
  91. 4:01plating is about 20 times stronger than
  92. 4:04the plastic resins and about 50 times
  93. 4:06stiffer. So, we change the mechanical
  94. 4:08properties substantially.
  95. 4:10I wanted to briefly interrupt here
  96. 4:12because Shawn shared a video outlining
  97. 4:15Repl's electroplating process. It's very
  98. 4:18insightful. So, by playing it now, it'll
  99. 4:21help make the rest of the conversation
  100. 4:23make a bit more sense. Let's check it
  101. 4:25out.
  102. 4:25>> After printing, the parts are removed
  103. 4:27from the platform and rinsed twice in
  104. 4:29IPA baths with a final spray rinse with
  105. 4:32clean IPA. The parts are then cured
  106. 4:35thoroughly and light cured to ensure
  107. 4:38there is no residual unccured resin,
  108. 4:40which will interfere with the
  109. 4:42metalization step.
  110. 4:44The lightweight parts with a high
  111. 4:46surface area
  112. 4:48use a loose hold on a rack so that parts
  113. 4:50can move while plating. After racking,
  114. 4:53the parts will be sprayed with a fine
  115. 4:54abrasive to provide a good edge for the
  116. 4:56conductive layer to adhere to. The
  117. 4:58metallization line is four process baths
  118. 5:01with each one followed by a rinse and
  119. 5:04deionized water. It starts with a soap
  120. 5:06solution to remove any residual soils
  121. 5:09from the earlier steps.
  122. 5:17The second bath is a mixed activator
  123. 5:19catalyst system that makes the surface
  124. 5:21of the part susceptible to autocatalytic
  125. 5:23nickel deposition.
  126. 5:31The third bath is an accelerator that
  127. 5:33complexes out the activator portion of
  128. 5:35the previous bath, making the final step
  129. 5:38in the process proceed more quickly.
  130. 5:47The final bath which is dark blue is the
  131. 5:49autocatalytic nickel deposition where 1
  132. 5:52microns of nickel phosphorus conductive
  133. 5:54layer is applied. The time to one rack
  134. 5:56through the four process and rinse tanks
  135. 5:59in this line is about 40 minutes.
  136. 6:06After a final rinse in DI water, the
  137. 6:08parts are dried and tested for
  138. 6:09electrical continuity to the rack. We do
  139. 6:12a 100% inspection for conductivity to
  140. 6:15ensure complete autocatalytic nickel
  141. 6:17coverage on the parts prior to
  142. 6:19electroplating.
  143. 6:20The first electroplating step is almost
  144. 6:23always a copper layer. The copper baths
  145. 6:25deposit at a rate of six or 12 microns
  146. 6:28per hour depending upon the type of
  147. 6:30copper we apply. The lattice cubes
  148. 6:32typically get 50 microns of copper. So
  149. 6:35run so they run a little over eight
  150. 6:36hours in this tank.
  151. 6:39The copper lattice cubes are removed
  152. 6:41from the acid copper tank at the
  153. 6:42prescribed time and rinsed.
  154. 6:51They are then placed in a nickel
  155. 6:52sulfamate tank with power connected.
  156. 6:56We apply a nickel layer on the lattice
  157. 6:59cubes which is 125 microns thick. It
  158. 7:02begins with a deposit from a ductal
  159. 7:03nickel bath followed by a layer of hard
  160. 7:05nickel. Deposition rate is six microns
  161. 7:08per hour.
  162. 7:14The rack coming out of the hard nickel
  163. 7:15band tank is rinsed thoroughly as this
  164. 7:18is the last step in the plating process.
  165. 7:23The lattice cubes are unrackcked after
  166. 7:25plating. Parts are weighed to confirm
  167. 7:28the average metal thickness prior to
  168. 7:29plating. The parts weigh about six grams
  169. 7:33and 175 microns of copper and nickel
  170. 7:35plating should increase their weight by
  171. 7:3725 or so grams, bringing the total
  172. 7:39weight of the parts to above 30 g. With
  173. 7:43that, they are strong enough so that
  174. 7:45[clears throat] people can stand on them
  175. 7:46without fear of breaking.
  176. 7:53The pretty materials that I was kind of
  177. 7:54looking at primarily is SLA. So, I'm
  178. 7:58looking at general purpose resins. Gravy
  179. 8:005 is what we have quite a lot of on hand
  180. 8:02just through our form four printer. And
  181. 8:05we also have some rigid 10K.
  182. 8:07>> The the plating on it works pretty well.
  183. 8:09And it seems that most of the business
  184. 8:11we're getting in the 10K is um mold
  185. 8:13inserts and things like that to make
  186. 8:14them last a little bit longer.
  187. 8:17>> Oh, wow. Okay. Very interesting. Yeah,
  188. 8:19we uh we recently had some experience
  189. 8:20with Rigid 10K mold inserts. We had not
  190. 8:23considered plating them though. But what
  191. 8:24happens is it can very easily get too
  192. 8:26hot. And if it gets too hot, then the
  193. 8:29resin, the injection molded resin can
  194. 8:31stick to the Rigid 10K and start picking
  195. 8:34out surface detail. The plating helps
  196. 8:36spread the heat a little bit. Doesn't
  197. 8:38reinforce it that well because there's
  198. 8:40the plating is usually only about 4,000
  199. 8:43thick and the parts are half an inch to
  200. 8:45an inch thick. But the detail areas will
  201. 8:48hold up better if the plating's on it.
  202. 8:50Our customers tell us that three to five
  203. 8:52times more parts can be made on the
  204. 8:54tools after they're plated.
  205. 8:56>> Oh wow. So the other material that I was
  206. 8:58thinking we have a fuse in our Dallas
  207. 9:00location. So maybe uh we could print Oh,
  208. 9:03we just run nylon 12 on that on that
  209. 9:05printer.
  210. 9:06>> And that's fine. We we run a lot of
  211. 9:07PA12. Um I would say the bulk of the
  212. 9:10stuff we see these days is MJF from the
  213. 9:12HP machines and it works pretty well.
  214. 9:15We've got a lot of data on reinforcing
  215. 9:17PA12 that's made by the MJF method and I
  216. 9:20know the form lab's properties of the
  217. 9:22printed parts are very very similar. Um
  218. 9:25they tend to be fairly dense. We will
  219. 9:26look at densities of printed parts
  220. 9:27really carefully when we're dealing with
  221. 9:29centered parts because if a part is
  222. 9:32nearly fully dense, like between 95 and
  223. 9:3698% dense, it's probably going to run
  224. 9:38just fine. If it's under 90% dense,
  225. 9:41we're probably going to have a lot of
  226. 9:42standing issues and problems with it.
  227. 9:43It's a very simple screening technique
  228. 9:45that you can do with a balance in about
  229. 9:4730 seconds. And the other thing too is
  230. 9:49with the SLS, the gray [clears throat]
  231. 9:51material works a lot better than the
  232. 9:53white material. So the white material
  233. 9:55doesn't give you as high a density as a
  234. 9:57gray material, which is kind of to be
  235. 9:59expected because it just absorbs more
  236. 10:01laser energy.
  237. 10:03>> Is there any issues with uh because I
  238. 10:05know Formlapse puts like carbon black to
  239. 10:07I guess add that coloration. Does that
  240. 10:10cause any issues with the plating
  241. 10:11process? Um, we don't really seem to
  242. 10:13There are a lot of people that send us
  243. 10:14parts that are dyed, whether it's carbon
  244. 10:16black or something else. It's It's not a
  245. 10:18problem. It all just coats. And the fact
  246. 10:21that there's like chopped carbon fiber
  247. 10:22in that material. That was another thing
  248. 10:24I was wondering if that because I just
  249. 10:26know of carbon's conductivity. I didn't
  250. 10:28know if that threw off anything in the
  251. 10:30plating process.
  252. 10:31>> It needed to be conductive to get it to
  253. 10:33plate. Although it's not good enough to
  254. 10:34plate without a conductive layer
  255. 10:36applied, but no, it doesn't interfere
  256. 10:37with anything at all.
  257. 10:39We have worked with the onyx materials
  258. 10:42that the Mark Forge plates. The Mark
  259. 10:44Forge actually plates a tighter part
  260. 10:47than and particularly with the Onyx than
  261. 10:49you get from most FDM printers. So, we
  262. 10:52actually don't do too badly when
  263. 10:55somebody sends us an FDM print made with
  264. 10:58Onyx that's been vapor smooth. It often
  265. 11:00does well enough by itself that we don't
  266. 11:02need to go through a sealing process
  267. 11:04because the vapor smoothing process
  268. 11:06seals it because it's a tighter
  269. 11:08structure than you normally get out of
  270. 11:09an FDM printer. Most other FDM prints,
  271. 11:13we really need to use a resin seal
  272. 11:15because they have much coarser pores
  273. 11:16that come to the surface in odd places.
  274. 11:19The Mark Forge prints, you know, you
  275. 11:21tend to have more of a of a racetrack
  276. 11:23type of reinforcement if you're doing
  277. 11:25the continuous fibers. the
  278. 11:28electroplating puts a lot of fibers
  279. 11:30right at the surface and so it basically
  280. 11:33brings back the bending properties so
  281. 11:36that they're at least as good as the as
  282. 11:38the tensil properties. So it's a it's a
  283. 11:40really nice complement to the uh to what
  284. 11:42you can do with the uh the fibers and to
  285. 11:44make a high tensil strength part.
  286. 11:47>> You wouldn't have to do any
  287. 11:48post-processing steps prior to plating
  288. 11:51uh like where you have to seal the
  289. 11:52surface or anything. Uh assuming
  290. 11:55>> it it does need to be made well. It does
  291. 11:57does need to be cleaned well because if
  292. 11:59the surfaces have a lot of powder on
  293. 12:01them, they're not going to metalize
  294. 12:02well. But that shouldn't be that
  295. 12:04difficult.
  296. 12:05>> When it comes to plating a chain mail
  297. 12:07like that, you have to hold it really
  298. 12:09loosely.
  299. 12:11>> And the copper is much more likely to in
  300. 12:15essence grow together and bond. Okay?
  301. 12:18>> So you you literally have to break it up
  302. 12:20periodically while it's plating. And
  303. 12:23then you go into the nickel tank and you
  304. 12:26still worry about that, but you can go
  305. 12:28about four times as long. It normally
  306. 12:31does not. If you can get it through the
  307. 12:32copper tank without sticking to itself,
  308. 12:34you'll get it through the nickel tank
  309. 12:35without too much difficulty.
  310. 12:37What really matters is the quality of
  311. 12:40the print and how well it's finished.
  312. 12:43So, if you want something that's
  313. 12:44polished, you're going to have to make a
  314. 12:46part that is probably printed at a
  315. 12:49maximum of 50 micron build layer
  316. 12:51thicknesses. You're going to have to
  317. 12:52sand it and get rid of all the layer
  318. 12:54lines and make certain the top layers
  319. 12:56are very smooth. And then we usually
  320. 12:59plate at least 100 microns to 150
  321. 13:02microns of copper. And our we have a
  322. 13:04bath that actually levels out the
  323. 13:06surface a little bit um to get a bright
  324. 13:08copper layer. And then the nickel layer
  325. 13:09is only for finish work about 25
  326. 13:12microns. So in other words, you're doing
  327. 13:14most of the work is being done in the
  328. 13:16copper tanks and there may still be a
  329. 13:18little bit of work afterwards.
  330. 13:20>> Understood. And so it sounds to me like
  331. 13:22any kind of defects or or or surface
  332. 13:24imperfections in the printed part is
  333. 13:26really going to be like amplified or
  334. 13:28it's really going to show through uh
  335. 13:30after. Okay. In fact, one of one of the
  336. 13:33difficulties we have, a lot of people
  337. 13:34like to spray parts with um bead
  338. 13:36blasting and it makes the surface dull
  339. 13:38and you don't see any of the flaws. As
  340. 13:41soon as you put particularly a bright
  341. 13:44layer of plating on, every single one of
  342. 13:46those flaws that was hidden comes come
  343. 13:48basically becomes really prominent
  344. 13:50because you go from a low contrast
  345. 13:52surface to a very high contrast surface
  346. 13:54when you play parts.
  347. 13:56>> So, I saw you had some bronze patina
  348. 13:58coating.
  349. 13:59>> Yeah. which is really just copper with a
  350. 14:01a bronze patina finish. So, it's it's
  351. 14:03relatively easy to do. We would give you
  352. 14:05probably a semi- bright copper layer and
  353. 14:07then um the bronze patina gets applied
  354. 14:10and usually gets might get highlighted
  355. 14:12with steel wool or something like that.
  356. 14:15>> Can you uh enlighten me a little bit on
  357. 14:17what the like patina application process
  358. 14:19looks like?
  359. 14:20>> For cold patas, which is what we have to
  360. 14:24work with when we're dealing with plated
  361. 14:25plastic parts, we use a gel that we
  362. 14:27wipe. We basically spread over the
  363. 14:29surface, but you can also buy the patina
  364. 14:31in a like you can have it in a liquid
  365. 14:34container and you literally dip the part
  366. 14:36in in the patina for a certain period of
  367. 14:38time and you hold it in there and you
  368. 14:42take it out and you you dry it off.
  369. 14:45Sometimes you have problems where you
  370. 14:46might get a little bit of skip and you
  371. 14:47have to go back and redo it, but um and
  372. 14:50then you would highlight it. There's
  373. 14:52probably maybe a little bit of pre-work
  374. 14:53that needs to be done. It's really not
  375. 14:55that hard to apply a patina. There may
  376. 14:57be a little bit of prep work up front to
  377. 14:59basically make it just a little bit
  378. 15:01rougher than we normally get out of the
  379. 15:02tank, but that shouldn't be that hard to
  380. 15:04do.
  381. 15:06That little cube, it will hold 1,800 lb
  382. 15:09in the orientation you show.
  383. 15:12>> And if you turn the tube sideways, it'll
  384. 15:14hold 800 lb.
  385. 15:15>> So,
  386. 15:16>> oh my gosh,
  387. 15:17>> it's and and that's about 10 times more
  388. 15:19than it would hold if you didn't plate
  389. 15:21it. It's c that kind of lattice where
  390. 15:24you have a very high surface to volume
  391. 15:26ratio and a very high volume fraction of
  392. 15:28metal and we can get into that later.
  393. 15:30You get some really big time
  394. 15:33strengthening. You know, we don't do a
  395. 15:35lot of lattice parts and we actually
  396. 15:36wish we did a lot more because we're
  397. 15:38printing and plating. It is probably
  398. 15:40easier than conventional parts. So, we
  399. 15:43really like them, but we're trying to
  400. 15:45get more people to try more latisy type
  401. 15:48of things. And um we're slowly get
  402. 15:50they're slowly coming around. We've done
  403. 15:52work with a topology optimized
  404. 15:55threepoint bend sample and
  405. 15:57[clears throat] we literally designed it
  406. 15:58so it had the same tensil strength. The
  407. 16:01material had the same tensil strength as
  408. 16:02DMLS aluminum.
  409. 16:04>> Oh wow.
  410. 16:04>> And then and then when we broke a plated
  411. 16:08part this a very high metal volume
  412. 16:11fraction or the content was around I'd
  413. 16:13say 35% or so. It had it was actually
  414. 16:17twice as strong as the DMLS aluminum
  415. 16:18piece. And the reason for that was all
  416. 16:21the reinforcement is out on the surface.
  417. 16:24Whereas the DMLS aluminum piece, even
  418. 16:26though it has the same tensil strength,
  419. 16:28the reinforcement is uniform across the
  420. 16:31you know the it's a uniform tensil
  421. 16:33strength. So the I think the DMLS
  422. 16:34aluminum would has a tensil strength of
  423. 16:3750,000 PSI, but in bending you've got
  424. 16:39surface loads and the surface
  425. 16:41reinforcing layer is about 150,000 PSI.
  426. 16:44So, you actually get a better result
  427. 16:46with a plated plastic part.
  428. 16:48>> The the core of that plastic part that
  429. 16:50was plated, was it was it an SLA part?
  430. 16:53>> SLA clear resin standard stuff. Nothing
  431. 16:56special.
  432. 16:57>> Oh my gosh. So, not even like like a
  433. 16:59Ridge 10K or anything, just like your
  434. 17:01general purpose. That's
  435. 17:02>> what's funny is when you do when you
  436. 17:04have low volume fractions of metal on a
  437. 17:06part like you might with a housing
  438. 17:08that's got um let's say 1 millimeter
  439. 17:10walls and and maybe 75 microns of
  440. 17:13plating on it. The stiff materials
  441. 17:15really really do a lot better. When you
  442. 17:18get to 25 30% volume metal that stiff
  443. 17:23material doesn't help you very much
  444. 17:25anymore. the the metal is dominating and
  445. 17:27because a stiff material tends to
  446. 17:29fracture very easily and the tougher
  447. 17:32materials have a lot better elongation,
  448. 17:35they actually do a little bit better.
  449. 17:36And we've got data on that that we got
  450. 17:38with Form Labs that shows exactly that.
  451. 17:41If you have a high metal volume
  452. 17:42fraction, the coating has better strain
  453. 17:45capability than what's underneath it. So
  454. 17:48the rigid 10K breaks at the low volume
  455. 17:51fractions, they're working together.
  456. 17:53You'll often heard hear me talk about
  457. 17:55metal volume fractions because that's
  458. 17:57really how you need to be thinking about
  459. 17:59things and that's the the volume of
  460. 18:02metal versus the volume of plastic in
  461. 18:04the cross-section that's tested. That's
  462. 18:06how you predict what the parts are going
  463. 18:07to be.
  464. 18:08>> Yeah, that goes back to that rule of
  465. 18:10mixtures that you guys
  466. 18:11>> Yes, it does. It's exactly it.
  467. 18:13>> Okay. What are some of the applications
  468. 18:16where like abrasion resistance would
  469. 18:18would really be uh would really apply?
  470. 18:20Where the abrasion resistance matters is
  471. 18:23often when we are are dealing with parts
  472. 18:25that you know one thing slides against
  473. 18:27another or there may be abrasive
  474. 18:29particles coming through a tube or a
  475. 18:31pipe or something of that nature. And
  476. 18:33the way to get abrasion resistance is
  477. 18:36nearly all the work we do for
  478. 18:37strengthening uses electrolytic nickel
  479. 18:39because electrolytic nickel has good
  480. 18:42strength and good elongation. If you're
  481. 18:45after abrasion resistance, you need to
  482. 18:47use electroly nickel, which [snorts] is
  483. 18:49a nickel phosphorus material. And that
  484. 18:52material is twice as hard as
  485. 18:55electrolytic nickel. And it doesn't tend
  486. 18:59to gall the way nickel can when you have
  487. 19:02nickel sliding against itself because
  488. 19:04it's a harder surface. But you don't get
  489. 19:06much reinforcement from that electroly
  490. 19:08nickel. So, if you're making an abrasion
  491. 19:10resistant coating that needs to be and
  492. 19:12and you need a part that's also strong,
  493. 19:15what you do is you use you start with a
  494. 19:16regular copper layer as as your base
  495. 19:18layer, then you use the amount of
  496. 19:21electrolytic nickel you need to get the
  497. 19:23strength out of it and then you might
  498. 19:25put a top coat of maybe 25 microns of
  499. 19:28electrolytes nickel to give you the bra
  500. 19:29the abrasion resistance you're looking
  501. 19:31for. It's just a question of sequencing
  502. 19:33and putting that top layer on. And you
  503. 19:35probably need to be a little bit careful
  504. 19:36about sizes and the resins because when
  505. 19:40you're the electroly nickel is applied
  506. 19:42at 90° C whereas all the electrolytic
  507. 19:45work is done at under 45° C. And so it's
  508. 19:49you can probably get away with almost
  509. 19:51anything with electro blading. You're a
  510. 19:53little bit more limited when you get to
  511. 19:54the electrolyt materials particularly as
  512. 19:56you get larger parts.
  513. 19:58>> Okay, understood. Yeah. So it sounds
  514. 20:00like the uh you need like a higher
  515. 20:02performance resin if anything that can
  516. 20:04that can handle those temperatures.
  517. 20:06>> Well, you also want a low CTE resin and
  518. 20:09so that's actually one of the places
  519. 20:10where using a um a rigid 10K has real
  520. 20:14advantages since we don't run our
  521. 20:17electroly nickel that often and and we
  522. 20:19don't run large baths of electroly
  523. 20:21nickel. We tend to have to make it up
  524. 20:22and throw it out. So it does add cost.
  525. 20:24But if we had baths that we ran
  526. 20:26routinely, then the electrolist nickel
  527. 20:28wouldn't cost that much more to get that
  528. 20:30layer applied. How does a plated plastic
  529. 20:33do versus a printed copper piece? And in
  530. 20:37order to get good conductivity through a
  531. 20:38piece of copper, you really want to have
  532. 20:41all copper from one side to the other.
  533. 20:43[snorts] I would bet on the bottom of
  534. 20:45that plate there, it is um a solid
  535. 20:48copper piece. Then you have those other
  536. 20:50pieces rising up off of it. Well, if we
  537. 20:52had a plastic plate, we're pling over
  538. 20:54it. We now have an insulating layer. So,
  539. 20:57we would probably want that plate
  540. 20:59perforated. We'd probably want to run
  541. 21:01samples through it, but we're only going
  542. 21:02to get the conductivity that you'd get
  543. 21:03from the copper layer, which might only
  544. 21:06be, let's say, 150 micron thick, 6,000
  545. 21:08of an inch thick, and it's not going to
  546. 21:10probably work as well as as a solid
  547. 21:12copper piece.
  548. 21:14>> Logical conductivity is literally
  549. 21:16>> 20 magnitudes higher than it than the
  550. 21:18plastic is. But the thermal conductivity
  551. 21:22is three orders of magnitude higher. So
  552. 21:24it's you know you're it's going to help
  553. 21:27but you really need a high metal volume
  554. 21:29fraction to do a lot. But you all but
  555. 21:32remember because there's plastic there's
  556. 21:35going to be a path dependency that you
  557. 21:36we have to be very careful careful of
  558. 21:38and conscious of in the way the heat
  559. 21:40sink is designed.
  560. 21:43electroplating. Does it have the
  561. 21:45capacity to take a 3D printed part that
  562. 21:48is uh for the most part not food safe
  563. 21:51and to some degree not necessarily
  564. 21:53biocompatible? Is it capable of of
  565. 21:55achieving that level of uh of like
  566. 21:58certification and safety?
  567. 22:00>> Well, I know that there's electroplating
  568. 22:02of nickel that's used for food safe
  569. 22:05applications. I know that that occurs.
  570. 22:07It's mostly people plating on metals.
  571. 22:09[snorts] any specific reason why the
  572. 22:12core of the part be metal versus plastic
  573. 22:14for food?
  574. 22:15>> Probably the the number one thing is the
  575. 22:18bond to metal of of electroplated
  576. 22:21coating to metal is much much stronger
  577. 22:23than the bond of electroplated metal to
  578. 22:25plastic. Plastic just doesn't have the
  579. 22:27tensil strength even if you've got a
  580. 22:29decent bond. So the chances of something
  581. 22:31breaking or you could, you know, get
  582. 22:33delamination and get a blister and then
  583. 22:35that could lead to other problems. So it
  584. 22:37it probably has more to do with is the
  585. 22:41coating but what's the likelihood of the
  586. 22:42coating coming off the part and leading
  587. 22:45a to a contamination problem in the
  588. 22:47food. And that's really what what I
  589. 22:49think the issue is going to be. It is
  590. 22:51not going to be safe for uh somebody
  591. 22:53making a an implant or something like
  592. 22:56that. I think there's like a literally a
  593. 22:58handful of metals maybe um six to 10
  594. 23:01that you can use for implants and things
  595. 23:03like that. Chrome is one of them.
  596. 23:06stainless steel, which does contain some
  597. 23:08nickel, um, but but only certain alloys.
  598. 23:10Titanium,
  599. 23:12you know, you're really limited in what
  600. 23:13you can implant people with. There's
  601. 23:15about a third of the population has a
  602. 23:18has sensitivity to nickel and so it's
  603. 23:21it's not the sort of thing you can ever
  604. 23:23think about implanting at all. I mean,
  605. 23:25you can make prototypes and people can
  606. 23:27test out those prototypes, but they're
  607. 23:29not going to be an implantable item. I I
  608. 23:32saw that one of the coding options that
  609. 23:34you have was EMI like EMI shielding. I I
  610. 23:37would take it as
  611. 23:39>> that's a big part of our business. Okay.
  612. 23:41And normally it's not just copper. It's
  613. 23:43usually mostly copper with a little bit
  614. 23:45of nickel applied over it.
  615. 23:46>> Copper will oxidize over time. So a
  616. 23:49little layer of nickel prevents that.
  617. 23:50You know, you've got a box there that's
  618. 23:52got 3mm walls. And you can take that
  619. 23:55same box and make it 1 mm walls and now
  620. 23:59put a mill of copper which is what you
  621. 24:01need for your EMI shielding and then 2
  622. 24:03mls of nickel which you would need for
  623. 24:05strengthening. And now you might
  624. 24:07actually end up with a lighter box and
  625. 24:09that's um a lot more resilient. We do a
  626. 24:12lot of work with aerospace companies and
  627. 24:14it's rare to see an EMI shielding box on
  628. 24:18an aircraft that's going to fly,
  629. 24:20[snorts] you know, mostly drones and
  630. 24:22things like that. They're almost all one
  631. 24:23millimeter wall thickness parts and
  632. 24:26using at least equal parts of copper and
  633. 24:29nickel and sometimes twice as much
  634. 24:30nickel as copper.
  635. 24:32>> Oh wow. And and again this is for the
  636. 24:34shielding of any kind of interference.
  637. 24:36That's
  638. 24:36>> it's shielding but it's also
  639. 24:38strengthening of the part. So it's a
  640. 24:40it's a multifunctional coating which is
  641. 24:42not that hard to do when you're just
  642. 24:44going bath to bath.
  643. 24:46>> Are you seeing use cases for this stuff
  644. 24:48like on aircraft or is it primarily
  645. 24:51drones?
  646. 24:52from our understanding is most of these
  647. 24:54are for UAVs. And in all honesty, the
  648. 24:57UAV is a much better place to be these
  649. 25:00days than aircraft because we're
  650. 25:01spending a lot more money on drones than
  651. 25:04we're spending on aircraft. And the
  652. 25:05barriers to getting onto that aircraft
  653. 25:07are a lot smaller.
  654. 25:09>> I guess the FAA probably has a lot fewer
  655. 25:12restrictions on on what can go on a
  656. 25:14drone than what can go in an aircraft.
  657. 25:17anything with people in it, you've got
  658. 25:19to be really, really careful and you're
  659. 25:20going to go through all kinds of
  660. 25:22certifications.
  661. 25:24>> You're making a drone or particularly
  662. 25:25even a one-way piece,
  663. 25:27>> you know, you've got latitude that you
  664. 25:29just don't have. And that's why saying
  665. 25:31the barriers are lower to getting in and
  666. 25:34the applications are numerous
  667. 25:36>> and the [clears throat] size of the
  668. 25:37parts is compatible with what you can
  669. 25:39print.
  670. 25:40So the the box on the right, you know,
  671. 25:44down here,
  672. 25:45>> that's a plated electrical box with one
  673. 25:47mil of copper, two mills of nickel, and
  674. 25:49then that's the unplated box on that's
  675. 25:51white behind it. And that's all made
  676. 25:53from rigid 4K.
  677. 25:56>> Okay. Terrific.
  678. 25:57>> And the rigid 4K one broke, but the ri
  679. 25:59but the plated one's doing just fine,
  680. 26:02>> I bet.
  681. 26:04Very nice.
  682. 26:06Sometimes it's relatively easy to take
  683. 26:08an antenna as it's designed. Other times
  684. 26:11people want to make a resident cavity
  685. 26:13where you basically have a closed box
  686. 26:15with a few openings in it here and
  687. 26:18there. In many cases, those are
  688. 26:20impossible to plate. And one of the
  689. 26:23things that we've had the opportunity to
  690. 26:25work with people who are very good
  691. 26:26antenna designers, they know how the way
  692. 26:30the antenna works. They know where you
  693. 26:32need material and when you don't need
  694. 26:33material. And then they take that
  695. 26:35antenna and they turn it into Swiss
  696. 26:39cheese in a way that it still functions
  697. 26:41properly as an antenna, but now it's
  698. 26:43really easy to plate. So, um, it's that
  699. 26:46kind of level of interaction between how
  700. 26:50the part really functions and what you
  701. 26:52can electroplate. In other words, when I
  702. 26:55talk to people about lattice structures
  703. 26:56or perforated structures, the probably
  704. 26:59the the the strangest thing that they'll
  705. 27:01hear from me is it's easier to plate a
  706. 27:04lattice structure than it is to plate a
  707. 27:05solid structure. With solid structures,
  708. 27:08you know, the wall thickness may be too
  709. 27:10thick. We may have to use supplemental
  710. 27:11anode. When you when you make a lattice,
  711. 27:14all of a sudden, all those problems go
  712. 27:16away.
  713. 27:17But uh like selectively masking areas is
  714. 27:20that's what what kind of goes in with
  715. 27:22that if it's even possible.
  716. 27:24>> What I'm going to say about selective
  717. 27:26work is what we do is we literally just
  718. 27:30tape off areas that need to be masked.
  719. 27:33[snorts]
  720. 27:33>> Okay.
  721. 27:34>> But on the other hand, if you can figure
  722. 27:36out how to do the masking
  723. 27:39or the selectivity
  724. 27:41in the printing process
  725. 27:44>> Mhm. that would make this really
  726. 27:46efficient and easy. Let's say you want
  727. 27:48an area that where you're going to be
  728. 27:50selectively, you know, having some
  729. 27:52circuits or something like that on it.
  730. 27:54Well, maybe all the circuits are
  731. 27:55recessed and then all the areas that are
  732. 27:57not to be plated will be raised. Then we
  733. 28:00could basically metalize everything with
  734. 28:02conductive layer. Don't plate it yet.
  735. 28:04And then remove all the height all the
  736. 28:07conductive layer off of the high spots.
  737. 28:09Then electroplating electroplate that
  738. 28:12and we have circuits. I think the key to
  739. 28:15making that selectivity work is do the
  740. 28:19selectivity in the printer because the
  741. 28:20printer is much more accurate than what
  742. 28:22people can do by hand. Uh
  743. 28:24>> best to send us files to to evaluate and
  744. 28:27we can give you a quote based upon files
  745. 28:30>> and would you prefer like step files or
  746. 28:32or something even
  747. 28:34>> STL files are preferred but we can we
  748. 28:36can we can deal with steps too if that's
  749. 28:38all you have. We do a lot of parts that
  750. 28:41have to fit together and a lot of times
  751. 28:44people will design the parts you know
  752. 28:46just to be printed and that's you know
  753. 28:48the end of it. When we start adding
  754. 28:51layers to it we're going to create
  755. 28:52interferences
  756. 28:54but with STL files or with step files
  757. 28:57it's very easy to offset surfaces
  758. 28:59inwards to make room for the coating.
  759. 29:01And we believe very very strongly that
  760. 29:04the process starts before you even print
  761. 29:07the part because you need to understand
  762. 29:09how much material you need for the job
  763. 29:11you're doing and then you have to modify
  764. 29:14the file before you print it. That's
  765. 29:17really essential to make this work well.
  766. 29:20I know uh you've talked about like screw
  767. 29:22threading before that one is a a
  768. 29:25>> for for small parts you're you're going
  769. 29:27to do screw threading with you know
  770. 29:29either inserts or something of that
  771. 29:31nature. But for let's say for a large
  772. 29:33part where you have um you know a 2in um
  773. 29:39uh let's say a 2in diameter you know
  774. 29:42pipe or something like that where it
  775. 29:44just got to you know screw together.
  776. 29:46You're going to need the offsets on the
  777. 29:47surfaces to make those work.
  778. 29:49And it's not hard, but you better plan
  779. 29:52for it or you're going to be basically
  780. 29:54driving yourself nuts trying to fix it.
  781. 29:57>> Thanks again to Sean and his team at
  782. 29:59Replform taking the time to uncover all
  783. 30:02the secrets of electroplating 3D printed
  784. 30:04parts. There's some incredibly useful
  785. 30:07information here that you can reference
  786. 30:08back to as you take on your next
  787. 30:10electroplating project.

About this transcript

This page contains the full transcript of Plastic In. Metal Out. | Electroplating 3D Printed Parts for Metal Performance (Part 1) by MLC CAD Systems, generated from the public captions YouTube serves with the video. The transcript has 5,297 words across 787 segments, with the original timestamps preserved so you can click any line to jump to that moment in the embedded player.

What you can do with it

Use the transcript to take notes, quote the speaker, build a study guide, generate a summary with ChatGPT or Claude via the YouTube Summary tool, or export it as a timed subtitle file with YouTube to SRT. You can also re-open it in the transcriber to choose a caption track available on the video.

Free YouTube transcript tool

YouTube2Text is a free YouTube transcript generator — no signup, no daily limit. Paste any YouTube link and get the full transcript instantly, with timestamps, click-to-jump, caption language selection, AI prompts for ChatGPT, Claude, and Gemini, and exports to TXT, SRT, VTT, or Markdown.